YBCO growth

The most complex process is YBCO growth. That process is described here.

Switch off the pumps

  1. Check whether all gas inlet valves are closed
  2. Close the gate valve
  3. Switch off the pumps with the central pump switch
  4. Switch off the cooling water

Open the chamber

  1. Vent the chamber by opening the N2 chamber valve and turning the gas selector valve to N2
  2. Close both valves when the pressure is 8e2 Torr.
  3. Switch on the Lift main switch
  4. Raise the top of the system using the lift control unit and rotate the top to the left.

Mount the substrate

  1. ALWAYS wear gloves when touching substrates and system parts
  2. Remove the heater shield
  3. Remove samples, clean sideplates in HNO3
  4. Clean the heater surface 1)with a razor, 2)with 400 grit sandpaper, 3) with 800 grit sandpaper, 4) with Scotchbrite. Clean with IPA. This step is crucial!
  5. Mount the sample with SPI silver paste plus II (should be kept in freezer, warm up before use) and squeeze the substrate against the heater with the glass tool (clean before use)
  6. Shine a halogene lamp on the substrate for 15 minutes
  7. Cut away glue around the substrate
  8. Mount side plates, push them flush against the substrate using a cotton tip.
  9. Set the heater to 80 C for 1 hour using the Eurotherm control software
  10. Dry for >1 hour
  11. Mount the heater shield, blow possible dust particles away with N2

Close the chamber

  1. Rotate the top above the chamber and lock it in place
  2. Lower the top very carefully making sure that the teflon guides slide along the chamber (take into account safety rules for working with heavy objects)
  3. Switch off the lift main switch

Pump down

  1. Open the gate valve
  2. Switch on diaphragm pump
  3. Wait until the pressure is about 5 torr on the pirani or 8 mbar on the capacitance gauge
  4. Switch on cooling water
  5. Switch on turbo
  6. At 800 Hz: open main gas valve under the chamber
  7. Check that the ion gauge switches on
  8. Pump overnight

Deposition

Procedure start
  1. Pressure should be 1e-6 mbar
  2. Position heater between 2 sources, opposite to YBCO
  3. Open N2 purge on the pump. Do not forget this!
  4. Open the O2 valve at the front of the system. Do not touch the O2 needle valve! Flow should be around 40.
  5. Open the YBCO shutter, keep other shutters closed (unless you make a multilayer of course)
  6. Switch on the YBCO power supply, current regulation
  7. Set the setpoint at 8 ma, display actual current and voltage
  8. Switch turbo to pressure control, setpoint 3.5
  9. Short after that, when the pressure is between 5e-2 and 1e-1 torr, switch power supply to on. The plasma should ignite. Get help if it doesn't!
  10. Let the pressure increase until the voltage gets below 350-380 V (the lower the better!)
  11. The voltage keeps decreasing, keep it constant at 350-380 V by increasing current (it is critical that you follow this rate given by the O2 backfill rate of the chamber and not faster!
  12. The turbo pump is at 0 Hz now and starts to accelerate
  13. At 100 Hz, set pressure setpoint to previous value from the logbook
  14. Keep increasing current, set current to 350 mA (never get above 390 V!)
  15. Use the Keithley to read O2 pressure, fine adjust setpoint so that pressure is between 2.99 and 3.01 mbar (better: 2.995 - 3.005)
  16. Let everything stabilize
Presputtering
  1. You will see that the conditioning of the target takes quite a while, check that while conditioning the voltage goes down to about the previous value in the logbook.
  2. Presputter for >1 hour
  3. Program the heater in the meanwhile. There is a recipe for YBCO.
Sputtering
  1. Run the recipe
  2. When the deposition substrate temperature is reached, the temperature will overshoot 2 or 3 degrees. Get ready to rotate the substrate above the YBCO source.
  3. Immediately (absolutely do not wait) when the temperature is right (0-1 degree from the setpoint) rotate the target above the source. Check the symmetry of the plasma and the substrate position. Start a timer.
  4. Time the epitaxial growth process
Annealing
  1. Turn the substrate away and press Skip segment on the Eurotherm control program
  2. Turn off the power supply and turn the setpoint back
  3. Set the chamber backfill selector to O2
  4. Wait until the substrate reaches the annealing temperature + 10 degrees
  5. Quickly close the gate valve and the O2 valve
  6. Close the gas valve under the chamber and exactly at the annealing temperature open the chamber backfill valve (you have to be quick here!)
  7. Close the chamber backfill valve at 8e2 torr (reproduce this value!)
  8. Set the chamber backfill gas selector to neutral

End

  1. Let pump run for 20 minutes
  2. Close N2 purge on the pump.
  3. The Eurotherm control program takes the sample trough the annealing temperature profile
  4. Wait until the sample temperature is <50 C
  5. Check whether all gas valves are closed